Soft X-ray resonant magnetic scattering from a Ni layer with modulated magnetic anisotropy

CROSSMARK_Color_square_no_text.svg

aMagnetic Spectroscopy, Daresbury Laboratory, Warrington WA4 4AD, UK, bInstitute of Low Temperature and Structure Research, Polish Academy of Science, PO Box 1410, Wroclaw, Poland, cDiamond Light Source Ltd, Rutherford Appleton Laboratory, Didcot, Oxon OX11 0QX, UK, dCavendish Laboratory, University of Cambridge, Madingley Road, Cambridge CB3 0HE, UK, and eEuropean Synchrotron Radiation Facility, BP 220, F-38043 Grenoble, France
*Correspondence e-mail: g.van_der_laan@dl.ac.uk

(Received 16 November 2003; accepted 2 March 2004)

Soft X-ray resonant magnetic scattering studies on a magnetically modulated, but nominally chemically homogenous, 5 nm Ni layer in a Cu/Ni/Cu/Co/NiO/GaAs(110) system are reported. It was possible to estimate the main chemical structure of the sample on the basis of the results from specular reflectivity and rocking scans, probing the scattering vector components in the perpendicular and in-plane direction to the Ni wires, respectively. The magnetic scattering using polarized X-rays demonstrates the magnetic modulation of the Ni layer.

1. Introduction

In the pursuit of ever-increasing ultrahigh-density storage capabilities, the size dependence of the spin configurations and reversal processes of magnetic nanostructures produced by lithographic patterning of thin magnetic films are of significant scientific and technological interest. While isolated `island' magnetic structures, such as dots, wires and other special geometries, have already been studied (Dürr et al., 1999[Dürr, H. A., Dudzik, E., Dhesi, S. S., Goedkoop, J. B., van der Laan, G., Belakhovsky, M., Mocuta, C., Marty, A. & Samson, Y. (1999). Science, 284, 2166-2168.]; Dudzik et al., 2000[Dudzik, E., Dhesi, S. S., Dürr, H. A., Collins, S. P., Roper, M. D., van der Laan, G., Chesnel, K., Belakhovsky, M., Marty, A. & Samson, Y. (2000). Phys. Rev. B, 62, 5779-5785.]; Jaouen et al., 2002[Jaouen, N., Tonnerre, J. M., Raoux, D., Bontempi, E., Ortega, L., Muenzenberg, M., Felsch, W., Rogalev, A., Dürr, H. A., Dudzik, E., van der Laan, G., Suzuki, M. & Maruyama, H. (2002). Phys. Rev. B, 66, 134420/1-14.]; Chesnel et al., 2002[Chesnel, K., Belakhovsky, M., Landis, S., Toussaint, J. C., Collins, S. P., van der Laan, G., Dudzik, E. & Dhesi, S. S. (2002). Phys. Rev. B, 66, 024435/1-9.]), the experimental realisation of patterned magnetic structures in a nominally chemically homogeneous film remains an important goal. Controlling both the intrinsic properties of the material and the sample dimensions of the magnetic domains in continuous films can open up new avenues for fundamental studies and device applications. Such structures can be used as a planar patterned magnetic medium, without breaking the homogeneity of the magnetic film which avoids reduced Curie temperature effects (Cowburn et al., 1997[Cowburn, R. P., Adeyeye, A. O. & Bland, J. A. C. (1997). Appl. Phys. Lett. 70, 2309-2311.]). It also introduces a new way of controlling spin configurations instead of stabilizing the natural domains (Krusin-Elbaum et al., 2001[Krusin-Elbaum, L., Shibauchi, T., Argyle, B., Gignac, L. & Weller, D. (2001). Nature (London), 410, 444-446.]). Locally controlled spin configurations do not have lateral dimension limitations and thus provide a reproducible switching mechanism, unlike geometrically restricted domains (Taniyama et al., 1999[Taniyama, T., Nakatani, I., Namikawa, T. & Yamazaki, Y. (1999). Phys. Rev. Lett. 82, 2780-2783.]; Ebels et al., 2000[Ebels, U., Radulescu, A., Henry, Y., Piraux, L. & Ounadjela, K. (2000). Phys. Rev. Lett. 84, 983-986.]).

Recently, Li et al. (2002[Li, S. P., Lew, W. S., Bland, J. A. C., Lopez-Diaz, L., Vaz, C. A. F., Natali, M. & Chen, Y. (2002). Phys. Rev. Lett. 88, 087202/1-4.]) and Bland et al. (2002[Bland, J. A. C., Lew, W. S., Li, S. P., Lopez-Diaz, L., Vaz, C. A. F., Natali, M. & Chen, Y. (2002). J. Phys. D, 35, 2384-2390.]) demonstrated a novel approach to controlling the magnetic structure in chemically homogenous films via the artificial modification of substrate surface properties prior to growth. Selective epitaxial growth introduces an alteration between single-crystal and polycrystalline structures in the film, according to the substrate patterning. The modulated single-crystal/polycrystalline substrate surface was used to locally modify the magnetic anisotropy in the subsequently deposited magnetic Ni film, which induces the desired magnetic structure. The well studied Cu/Ni/Cu(001) system was used to obtain domains with perpendicular magnetic anisotropy (PMA), which is attributed to the magnetoelastic interaction induced by the Ni/Cu(001) single-crystal interface (O'Brien & Tonner, 1994[O'Brien, W. L. & Tonner, B. P. (1994). Phys. Rev. B, 49, 15370-15373.]), while in the polycrystalline Ni domains the magnetization lies in the film plane owing to the dominant demagnetizing field.

X-ray reflectivity provides a routine method of gathering structural information, such as layer thickness, effective electron density and interfacial roughness (Daillant & Gibaud, 1999[Daillant, J. & Gibaud, A. (1999). X-ray and Neutron Reflectivity: Principles and Applications, Lecture Notes in Physics 58. Berlin: Springer.]; Als-Nielsen & McMorrow, 2000[Als-Nielsen, J. & McMorrow, D. (2000). Elements of Modern X-ray Physics. New York: Wiley.]). However, the capabilities of conventional X-ray reflectivity are limited when it is necessary to distinguish between the structural parameters from layers of neighbouring elements in the periodic table, such as Co, Ni and Cu, as in the case of our system (see Fig. 1[link]). A way of enhancing the chemical contrast is to take advantage of the tunability of the incident photon energy, which has become possible with the advent of synchrotron radiation (Kao et al., 1994[Kao, C.-C., Chen, C. T., Johnson, E. D., Hastings, J. B., Lin, H. J., Ho, G. H., Meigs, G., Brot, J.-M., Hulbert, S. L., Idzerda, Y. U. & Vettier, C. (1994). Phys. Rev. B, 50, 9599-9602.]; Tonnerre et al., 1998[Tonnerre, J. M., Sève, L, Barbara-Dechelette, A., Bartolomé, F., Raoux, D., Chakarian, V., Kao, C. C., Fischer, H., Andrieu, S. & Fruchart, O. (1998). J. Appl. Phys. 83, 6293-6295.]; Sève et al., 1999[Sève, L., Jaouen, N., Tonnerre, J. M., Raoux, D., Bartolomé, F., Arend, M., Felsch, W., Rogalev, A., Goulon, J., Gautier, C. & Bérar, J. F. (1999). Phys. Rev. B, 60, 9662-9674.]). The scattering factor will be enhanced near the absorption edges of the various elements in the sample. This resonant enhancement can be used to tune into the element-specific scattering cross section and to increase the sensitivity to the structural features. For 3d transition metals we use the excitation of 2p electrons into unoccupied 3d states resulting in strong absorption edges with energies in the soft X-ray region (van der Laan & Thole, 1991[Laan, G. van der & Thole, B. T. (1991). Phys. Rev. B, 43, 13401-13411.]).

[Figure 1]
Figure 1
Schematic of the measured sample Cu (5 nm)/Ni (5 nm)/Cu (70 nm)/Co (1.8 nm)/NiO (1 nm)/GaAs(110). The thickness of the layers is given according to the characterization by Li et al. (2002[Li, S. P., Lew, W. S., Bland, J. A. C., Lopez-Diaz, L., Vaz, C. A. F., Natali, M. & Chen, Y. (2002). Phys. Rev. Lett. 88, 087202/1-4.]). Polycrystalline and single-crystalline regions of the sample are indicated by PC and SC, respectively. Also shown are the experimental scattering geometries for (A) X-rays perpendicular to the wires and (B) X-rays parallel to the wires.

In this paper we will present soft X-ray resonant magnetic scattering (SXRMS) results on the Cu/Ni/Cu system in which the Ni layer has a wire pattern of modulated magnetic anisotropy (Fig. 1[link]). Since the properties of the sample are closely related to the structure, we demonstrate that SXRMS is a chemical-structure- and magnetic-structure-sensitive and element-specific technique, which shows a large potential to study such complex magnetic systems. Very few SXRMS studies have been reported so far on artificially patterned magnetic samples (Chesnel et al., 2001[Chesnel, K., Belakhovsky, M., Landis, S., Rodmacq, B., Dudzik, E., Collins, S. P., Dhesi, S. S. & van der Laan, G. (2001). IEEE Trans. Magn. 37, 1661-1663.], 2002[Chesnel, K., Belakhovsky, M., Landis, S., Toussaint, J. C., Collins, S. P., van der Laan, G., Dudzik, E. & Dhesi, S. S. (2002). Phys. Rev. B, 66, 024435/1-9.]) and it is primarily the purpose of the current paper to demonstrate the potential of the technique, rather than to indulge in a detailed theoretical analysis of the scattering results.

2. Sample preparation

Using GaAs(001) as a substrate, a pattern was prepared of a wire array of width 2 µm and separation 4 µm, as described by Li et al. (2002[Li, S. P., Lew, W. S., Bland, J. A. C., Lopez-Diaz, L., Vaz, C. A. F., Natali, M. & Chen, Y. (2002). Phys. Rev. Lett. 88, 087202/1-4.]) and Bland et al. (2002[Bland, J. A. C., Lew, W. S., Li, S. P., Lopez-Diaz, L., Vaz, C. A. F., Natali, M. & Chen, Y. (2002). J. Phys. D, 35, 2384-2390.]). A schematic is shown in Fig. 1[link]. The pattern was obtained by optical lithography and a subsequent lift-off of 1 nm-thick Ni. The ultrathin pattern was then oxidized in air to become an ultrathin NiO pattern. The patterned substrate was annealed at 773 K for 2 h before film growth at room temperature. Continuous films of Cu(5 nm)/Ni(5 nm)/Cu(70 nm)/Co(1.8 nm) were deposited onto the substrate in UHV using molecular beam epitaxy. The 1.8 nm-thick Co is used as a seed layer to promote epitaxial growth on the GaAs substrate. The thickness of 5 nm for the Ni layer is chosen in order to obtain a strong PMA (O'Brien & Tonner, 1994[O'Brien, W. L. & Tonner, B. P. (1994). Phys. Rev. B, 49, 15370-15373.]), and the 5 nm-thick Cu overlayer is used to prevent oxidation. While the films grown on the ultrathin NiO patterns are polycrystalline, those grown directly onto the GaAs surface are single-crystal films. The results have been confirmed by in situ reflection high-energy electron diffraction (RHEED) analysis. Magneto-optical Kerr effect (MOKE) measurements were performed to obtain the hysteresis loops. While magnetic force microscopy (MFM) was used to study the magnetic domain structures, atomic force microscopy (AFM) was used to examine the sample surface (Li et al., 2002[Li, S. P., Lew, W. S., Bland, J. A. C., Lopez-Diaz, L., Vaz, C. A. F., Natali, M. & Chen, Y. (2002). Phys. Rev. Lett. 88, 087202/1-4.]; Bland et al., 2002[Bland, J. A. C., Lew, W. S., Li, S. P., Lopez-Diaz, L., Vaz, C. A. F., Natali, M. & Chen, Y. (2002). J. Phys. D, 35, 2384-2390.]). Using these combined methods one can characterize the magnetic structure of the sample, and using the RHEED technique one can confirm the coexistence of polycrystalline and single-crystal regions in the Ni layer. However, in order to reveal the internal structure of the system, a depth-sensitive probe, such as SXRMS, is required.

3. X-ray magnetic scattering

The SXRMS measurements were performed on beamline ID08 at the European Synchrotron Radiation Facility (ESRF) in Grenoble using the six-circle ultrahigh-vacuum diffractometer (Dhesi et al., 2004[Dhesi, S. S., Mirone, A., De Nadai, C., Ohresser, P., Bencok, P., Brookes, N. B., Reutler, P., Revcolevschi, A., Tagliaferri, A., Toulemonde, O. & van der Laan, G. (2004). Phys. Rev. Lett. 92, 056403/1-4.]). Synchrotron radiation with linear and circular polarization in the energy region between 700 and 950 eV was employed at grazing-incidence angles θ between 0.1 and 22.5°. The scattered X-rays were detected using a photodiode (mounted behind a rectangular aperture) in vertical geometry. For the magnetic characterization the sample magnetization was applied parallel to the wires using an in-plane magnetization coil providing a field up to 50 mT. Since the coercive field of the sample is 20 mT, this is sufficient to saturate the sample.

Two different types of scans were employed, namely rocking scans and reflectivity scans, which in reciprocal space measure the scattering signal along qx and qz, respectively (see Fig. 2[link]). Here, qz is the component perpendicular to the surface, while qx is the component of the scattering vector in-plane with the sample surface and perpendicular to the wires. The real-space geometries A and B used for rocking scans and reflectivity scans, respectively, are schematically illustrated in Fig. 1[link], and below we will describe these scans to improve the understanding of the experimental results given in this paper.

[Figure 2]
Figure 2
The reciprocal plane (qx, qz) showing the specular rod (qx = 0) and the equidistantly spaced diffraction rods ([\Delta{q_x}] = 0.0001 Å-1 for our sample). The qx scans (rocking scans) for [2\theta] = 4° and 12° at the Ni L3 resonance ([\lambda] = 14.5 Å) are shown by the thick grey horizontal lines. The qz scan (specular scan) is along the specular rod (qx = 0) as shown by the thick black vertical line. The grey areas indicate the inaccessible region.

3.1. qx scan with fixed 2θ (rocking scan)

The scattering is measured as a function of qx using a transverse scan with the scattering plane perpendicular to the wires (geometry A in Fig. 1[link]) by rocking the sample at a fixed detector position. This rocking scan provides information about the in-plane periodicity of the charge and/or magnetic configuration. The scan can be perceived as a so-called grating scan with fixed 2θ.

For ingoing grazing angle ([\theta+\alpha]) and outgoing grazing angle ([\theta-\alpha]) we obtain the components of the scattering vector as

[q_x=(4\pi/\lambda)\sin\theta\sin\alpha,\eqno(1)]

[q_z=(4\pi/\lambda)\sin\theta\cos\alpha,\eqno(2)]

where [\lambda] is the wavelength of the incident radiation and [\alpha] is the rocking angle, i.e. the angle between the scattering vector [{\bf{q}}] and the surface normal. The wavevector transfer [{\bf{q}}] = [{\bf{k}}-{\bf{k}}'] is the difference between the wavevectors [{\bf{k}}] and [{\bf{k}}'] of the ingoing and outgoing X-rays, respectively. Thus the rocking scan describes a circle in reciprocal space given by

[|{\bf{q}}|=\left(q_x^2+q_z^2\right)^{1/2}=(4\pi/\lambda)\sin\theta,\eqno(3)]

[q_z/q_x=\cot\alpha.\eqno(4)]

In our case the incident angle and rocking angle are small, so that equations (1)[link] and (2)[link] simplify to [q_x\simeq4\pi\theta\alpha/\lambda] and [q_z\simeq4\pi\theta/\lambda]. Thus, with fixed 2θ, the rocking scan measures the scattering intensity along the qx direction at constant qz.

Fig. 2[link] illustrates the reciprocal space map showing the specular rod and the equidistantly spaced diffraction rods, corresponding to our patterned sample. The horizontal lines at qz = 0.03 and 0.09 Å-1 represent the qx scans with 2θ = 4° and 12°, respectively, for a wavelength [\lambda] = 14.5 Å corresponding to the Ni L3 resonance. Access in reciprocal space is restricted by the horizon condition, [|\alpha|\le\theta], to the region on the map satisfying

[q_z^2\ge(4\pi/\lambda)|q_x|-q_x^2.\eqno(5)]

3.2. qz scan (specular scan)

The reflectivity is measured as a function of qz using a [\theta]–2[\theta] scan with the scattering plane parallel to the wires (geometry B in Fig. 1[link]). Specular reflection results in qx = 0 and qz = [(4\pi/\lambda)\sin\theta]. The specular scan, where qz is varied by scanning [\theta] and 2[\theta], provides information about the structural and magnetic depth profile of the sample. In the reciprocal space map of Fig. 2[link], the qz scan is shown by the vertical line (qx = 0).

4. Resonant enhancement

The huge enhancement in the scattering intensity across the Ni resonance is illustrated in Fig. 3[link], which shows the energy dependence of the scattering intensity measured using a qx scan with 2[\theta] = 10°. A strong intensity increase is observed at the energies of the Ni L3 and L2 edges, located at 852 and 870 eV, respectively. The presence of many higher-order diffraction peaks in the rocking scan shows that the patterned sample diffracts as a grating.

[Figure 3]
Figure 3
Two-dimensional plot of the photon-energy- and qx-dependence of the scattered intensity measured by rocking scans with 2[\theta] = 10° across the Ni L2,3 resonance.

Using polarized X-rays the resonant scattering becomes sensitive to the magnetic order of the sample (van der Laan, 1999[Laan, G. van der, Dürr, H. A., Dudzik, E., Roper, M. D., Collins, S. P., Hase, T. P. A. & Pape, I. (1999). Synchrotron Rad. News, 12(3), 5-9.]). By tuning the energy to the core resonance the weak magnetic signal can be increased by orders of magnitude when the magnetic orbitals are directly involved in the electric dipole transition, such as the [2p\to3d] excitation in first-row transition metals. The energy-dependent scattering amplitude fi for coherence resonant magnetic scattering can be written, to first order in the magnetization, as

[f_i(\omega)=(\boldvarepsilon'{^{\ast}}\cdot\boldvarepsilon)F^{\,0}-i\,(\boldvarepsilon'{^{\ast}}\!\times\!\boldvarepsilon)\cdot\hat{\bf{M}}_i\,F^{\,1},\eqno(6)]

where [\varepsilon] ([\varepsilon']) is the unit polarization vector of the incident (scattered) X-ray beam, [\hat{\bf{M}}_i] is the magnetization unit vector of the i-th site, and F0 and F1 are the charge and magnetic part of the resonance amplitude (Hannon et al., 1988[Hannon, J. P., Trammell, G. T., Blume, M. & Gibbs, D. (1988). Phys. Rev. Lett. 61, 1245-1248.]). The first term in equation (6)[link] has the same appearance as the non-resonant Thomson scattering, while the second term is unique to the resonance. The polarization dependence, given by the vector products, is of great benefit to determine the alignment of the magnetic moments. With [\sigma]-polarized light (i.e. linear polarization perpendicular to the scattering plane) one probes the charge due to [\sigma\to\sigma'] scattering and also the magnetization component (along [{\bf{k}}']) in the scattering plane due to [\sigma\to\pi'] scattering (van der Laan et al., 2000[Laan, G. van der, Dudzik, E., Collins, S. P., Dhesi, S. S., Dürr, H. A., Belakhovsky, M., Chesnel, K., Marty, A., Samson, Y. & Gilles, B. (2000). Physica B, 283, 171-174.]). With circularly polarized light one probes magnetic components both within and perpendicular to the scattering plane. If the difference signal between left- and right-circularly polarized light is taken to examine the magnetization, then only the component within the scattering plane and perpendicular to qz contributes to the magnetic signal. Also, helical and chiral magnetic structures, although not considered in this paper, can give magnetic scattering peaks (Dürr et al., 1999[Dürr, H. A., Dudzik, E., Dhesi, S. S., Goedkoop, J. B., van der Laan, G., Belakhovsky, M., Mocuta, C., Marty, A. & Samson, Y. (1999). Science, 284, 2166-2168.]).

The scattering intensity contains the modulus square of the amplitude [f_i(\omega)]. When the charge and magnetic periodicity is the same, there will be an overlap of the magnetic and charge peaks. Then, in order to study the magnetism one can sometimes exploit the interference between the two amplitudes which results in a change in the scattering signal upon reversal of the sample magnetization. Dichroic intensity changes of this type, upon reversal of either the circular polarization or magnetic vectors, scale with [({\bf{k}}+{\bf{k}}'\cos2\theta)\!\cdot\!{\hat{\bf{M}}}_i] (Lovesey & Collins, 1996[Lovesey, S. W. & Collins, S. P. (1996). X-ray Scattering and Absorption by Magnetic Materials. Oxford University Press.]).

5. Results and discussion

5.1. Structural profile of the sample

5.1.1. Element-specific depth structure

Although our main interest is the magnetic properties of the system, the chemical structure needs to be characterized first in order to evaluate the magnetic contribution. Fig. 4[link] shows qz scans measured at three different photon energies. They are remarkably different to each other. The soft X-ray wavelengths are too long (∼15 Å) to reveal Bragg scattering from atomic planes and, apart from their interfaces, the layers are expected to be homogeneous in depth. However, the scattered intensity still depends on the X-ray penetration depth, which is material dependent. It strongly varies with scattering angle and photon energy, especially near the critical angle and across the resonances. Intensity oscillations, known as Kiessig fringes, arise from the interference between the scattering amplitudes from the different layer interfaces. The periods of the Kiessig oscillations are inversely proportional to the layer thicknesses.

[Figure 4]
Figure 4
Specular rod scans (qz scans) at photon energies of 700 eV (below all relevant edges), 852.7 eV (at the Ni L3 edge) and 900 eV (just below the Cu L3 edge). The periods of the Kiessig fringes correspond to the layer thicknesses in reciprocal space.

At 700 eV, the photon energy is well below the Co, Ni and Cu L2,3 absorption edges, which means that the penetration depth is large enough for the X-rays to reach the substrate. The short-period oscillation observed on the qz scan at 700 eV (Fig. 4[link]) corresponds to a thickness of the Cu underlayer of 530 Å, which is smaller than the value of 700 Å estimated from the preparation method. By tuning the energy to the Ni L3 edges at 852.7 eV, the scattered intensity becomes sensitive to the Ni layer, and the long-period oscillation in Fig. 4[link] corresponds to a thickness of 70 Å. Owing to the increased absorption at the Ni edge the short-period oscillation related to the thick Cu underlayer is strongly suppressed. The thickness of the Cu capping layer was obtained from a measurement at 900 eV, which is just below the Cu L3 edge. Fig. 4[link] shows a short-period oscillation related to the thick Cu underlayer as well as an oscillation that is about ten times longer and corresponds to the Cu capping layer of 50 Å.

The patterned sample gives an additional feature in the reflectivity around qz = 0.05 Å-1 (Fig. 4[link]). Such a feature is normally not observed for a multilayer which is in-plane homogeneous. Therefore, we tentatively ascribe this strong dip at small qz value to the in-plane periodicity in the system. The NiO thin film pattern, the polycrystalline and single-crystal regions, the different oxidation for the top layers in the polycrystalline and single-crystalline regions will all act together as a diffraction grating. Scattered amplitudes from the different regions of the sample interfere owing to phase differences and might give rise to an additional variation in the scattered intensity.

5.1.2. In-plane structural profile

As already demonstrated by Fig. 3[link], the most direct way to extract information concerning the in-plane structure is by performing rocking scans. Figs. 5[link] and 6[link] show the qx scans measured with 2[\theta] = 4° and 12°, respectively, at different photon energies. The separation of [\Delta{q_x}] = 0.0001 Å-1 between the diffraction peaks, which are located around the specular reflection (qx = 0), corresponds to a wire periodicity that matches precisely the period of 6 µm, laid down by lithography.

[Figure 5]
Figure 5
The qx scans at [2\theta] = 4° measured at different photon energies.
[Figure 6]
Figure 6
The qx scans at [2\theta] = 12° measured at the photon energies of the Ni, Cu and Co L3 resonances. The curves have been offset for clarity. The arrows point at the shoulder visible at the left-hand side of the specular peak.

Fig. 5[link] shows the qx scans at 2[\theta] = 4°, which is near the critical angle of total reflection where the sampling depth is minimum. In this case the scattering will be strongly surface sensitive so that only the capping layer will contribute. Since AFM measurements did not reveal any correlated roughness on the surface (Li et al., 2002[Li, S. P., Lew, W. S., Bland, J. A. C., Lopez-Diaz, L., Vaz, C. A. F., Natali, M. & Chen, Y. (2002). Phys. Rev. Lett. 88, 087202/1-4.]), the appearance of first-order diffraction peaks suggest a different oxidation for the single-crystalline and polycrystalline regions of the Cu capping layer. It is also clear from Fig. 5[link] that the normalized intensity profile near the total-reflection angle is almost independent of the photon energy.

At increasing Bragg angles the penetration depth becomes larger, so that the scattering signal will gradually give more information about the buried layers. Fig. 6[link] shows the qx scans with 2[\theta] = 12°. As with the qz scans in Fig. 4[link], switching the photon energy changes the scattering signal depending on the scattering factors of the elements involved. The relative peak intensities as well as the peak shape depend on the specific photon energy and Bragg angle. The envelope function of the peak intensities gives the form factor, which can provide information about the average structure of the wires. When the photon energy is tuned to the Ni L3 or Cu L3 resonance, extra structure is observed in the specular peak, while also an additional shoulder appears on the left-hand side of each diffraction peak. We tentatively ascribe this to the interference between the scattered amplitudes of the grating profile at different depths in the sample. The peak shape of each diffraction peak is quite similar, and therefore can be considered as a structure factor that provides information about the periodicity of the pattern summed over the effective sampling depth. However, without any detailed calculations it is very difficult to assign the peak shape to particular structural features of the sample.

5.2. Magnetic modulation of the sample

The Ni layer is of main interest for the Cu/Ni/Cu magnetically modulated system. In order to be selective to the Ni layer and to obtain an optimal magnetic scattering cross section, the photon energy was tuned to the Ni L2,3 absorption edge. We will first demonstrate the presence of both in-plane and perpendicular magnetic domains in the Ni layer by using the magnetic direction selectivity of SXRMS. Thereafter, we report on the magnetic depth profile using the scattering angle and photon energy dependence of the magnetic circular dichroism (MCD) asymmetry ratio in specular reflectivity.

5.2.1. Coexistence of in-plane and perpendicular magnetic domains

The energy dependence of the specular reflectivity was measured across the Ni edges at 2[\theta] = 8° (i.e. qx = 0, qz = 0.06 Å-1) using [\sigma]-polarized light in geometry A. According to the vector product in equation (6)[link], [\sigma]-polarized light can detect the magnetization component in the scattering plane along [{\bf{k}}']. Since the scattering plane is perpendicular to the wires in geometry A (c.f. Fig. 1[link]), the magnetic scattering vanishes for the in-plane (parallel-to-wire) domains, and only the magnetic component perpendicular to the surface contributes to the magnetic scattering.

Fig. 7[link] shows the difference in scattered intensity from two different magnetic configurations of the sample. In the first configuration the sample is in remanence, where we expect it to contain both in-plane and perpendicular magnetic domains. In the second configuration all magnetic domains have been aligned in-plane along the wire direction using the magnetization coil. The difference between both configurations gives the magnetic signal from the domains with perpendicular magnetization. The non-zero difference signal shown in Fig. 7[link] proves the presence of domains with perpendicular magnetization. Unfortunately, we were not able to observe the much weaker first-order magnetic scattering, since the structural and magnetic periods overlap, resulting in charge and magnetic scattering peaks at the same position in reciprocal space. We also studied the magnetic behaviour of the sample using circular polarization in geometry B with the light helicity vector aligned either parallel or antiparallel to the magnetization of the wires, resulting in scattering signals denoted as I+ and I-, respectively. With circular polarization we observe differences between the scattering signals from the sample in remanence and with only in-plane magnetically aligned domains. Fig. 8[link] shows the asymmetry ratio (I+-I-)/(I++I-) for both types of magnetic configuration at 2[\theta] = 10° (i.e. qx = 0, qz = 0.076 Å-1). For the remanent sample the helicity vector of the circularly polarized light was reversed, while for the in-plane magnetically aligned domains the magnetization was reversed using the in situ magnetization coil. With circular polarization, both in-plane and perpendicular domains give a non-zero magnetic scattering. If the perpendicularly aligned magnetic domains remain unchanged, the contribution to the MCD in reflectivity will arise only from the reversal of the in-plane magnetic moments. For that reason the signal will be approximately twice as large for measurements with in-plane magnetic field than under remanence conditions, where in-plane and perpendicular magnetic moments coexist.

[Figure 7]
Figure 7
Specular reflectivity of the magnetic configuration in remanence (with coexisting in-plane and perpendicular magnetic domains) (black line) and the magnetic configuration with all magnetic moments aligned in-plane (thick grey line) together with the resulting difference spectrum (dashed line). The specular reflectivity was measured as a function of photon energy at [2\theta] = 8° using [\sigma]-polarized light.
[Figure 8]
Figure 8
Energy dependence of the asymmetry ratio (I+-I-)/(I++I-) in specular reflection at [2\theta] = 10° for the sample in remanence (dotted line) and with in-plane applied magnetic field (drawn line). The signal I+ (I-) is defined as the specular reflectivity with the sample magnetization aligned parallel (antiparallel) to the X-ray helicity vector.
5.2.2. Magnetic depth profile

The magnetic depth profile was studied using the scattering-angle- and photon-energy-dependence of the MCD asymmetry ratio in specular reflectivity (in geometry B). All results presented below are for the I+ and I- signals from the magnetic configuration in which all magnetic moments are aligned in-plane and are reversed using the magnetization coil.

Fig. 9[link] shows the dependence of the asymmetry ratio (I+-I-)/(I++I-) on the Bragg angle measured at the energies of the Ni L2 and L3 edges. The insert shows the difference signal (I+-I-), i.e. the MCD, shifted by +0.08. Because this difference signal varies strongly with Bragg angle and can also change sign, it is advantageous to present the scattering signal in the form of an asymmetry ratio. However, the short-period oscillations shown in the asymmetry ratio can also be produced by minima in the charge reflectivity. No magnetic signal is observed at [2\theta\le5^\circ], where the X-rays only penetrate the Cu capping layer. This proves that the capping layer is not magnetic. Strong changes in the reflectivity are observed at higher angles, clearly demonstrating the large sensitivity of the asymmetry ratio to the magnetic structure and magnetic interfaces.

[Figure 9]
Figure 9
The 2[\theta] dependence of the asymmetry ratio of the specular reflectivity at the photon energy of the Ni L3 (drawn line) and Ni L2 (dotted line) resonance. Note the strong reduction in amplitude of the Kiessig fringes for the Ni L3 resonance owing to the shorter absorption length at this stronger absorption edge. Insert: difference between the scattering signal with parallel and antiparallel applied magnetic field for the Ni L3 (drawn line) and Ni L2 (dashed line) resonance.

We have already presented in Fig. 8[link] (drawn line) the asymmetry ratio for in-plane magnetically aligned domains over the Ni L2,3 resonance in geometry B with 2[\theta] = 10°. In Fig. 10[link] we present a series of such energy scans for different Bragg angles at grazing incidence. Remarkably strong spectral changes can be observed as a function of the Bragg angle.

[Figure 10]
Figure 10
Photon energy dependence across the Ni L2,3 resonance for the sum signal (I++I-) (thick grey line) and the asymmetry ratio (I+-I-)/(I++I-) (thin black line) of the specular reflectivity measured for different grazing-incidence angles in geometry B. The signal I+ (I-) is defined as the specular reflectivity obtained by aligning the magnetization parallel (antiparallel) to the helicity vector of the X-rays.

The thick line in Fig. 10[link] gives the sum of the reflectivity signals (I++I-). The observed evolution of the sum reflectivity for different Bragg angles resembles that for the grazing-incidence reflectivity spectra of the thin NiO film (Alders et al., 1997[Alders, D., Hibma, T., Sawatzky, G. A., Cheung, K. C., van Dorssen, G. E., Padmore, H. A., Roper, M. D., van der Laan, G., Vogel, J. & Sacchi, M. (1997). J. Appl. Phys. 82, 3120-3124.]; van der Laan, 1999[Laan, G. van der (1999). J. Magn. Magn. Mater. 192, 297-304.]). This NiO film was measured with [\sigma]-polarization and the reflectivity results gave good agreement with an optical model calculation. Of course, our layer contains Ni metal, rather than NiO, which has a somewhat different Ni L2,3 multiplet structure. However, both systems show quite similar variations as a function of [\theta]; in particular there is a peak, consisting of several components, at both the L3 and L2 edge around [\theta] = 3°, which around [\theta] = 7° changes into a single peak at the L3 edge and disappears at the L3 edge. Also, the asymmetry ratios show a wealth of detailed structure, and the spectra in Fig. 10[link] are distinctly different from the reflectivity results on a Ni(110) crystal reported by Sacchi & Mirone (1998[Sacchi, M. & Mirone, A. (1998). Phys. Rev. B, 57, 8408-8415.]). The dichroic spectra in Fig. 10[link] can be regarded as an extension of X-ray magnetic circular dichroism (XMCD) in absorption (i.e. forward scattering). Compared with the absorption signal in XMCD, the scattering signal also includes the dispersive part of the scattering factor. The size of the dichroism in reflectivity can exceed that observed in XMCD. However, the energy dependence of the reflectivity (Fig. 10[link]) is more complicated than that of the XMCD. While the integrated signals in XMCD can be related to the orbital and spin magnetic moments (Thole et al., 1992[Thole, B. T., Carra, P., Sette, F. & van der Laan, G. (1992). Phys. Rev. Lett. 68, 1943-1946.]), this is much more difficult in the case of scattering. In order to apply the sum rules, the integral of the imaginary part of magnetic scattering factor would have to be extracted. However, the sum rules do not apply in the case of interference scattering where the charge scattering resonance varies with energy.

6. Summary

We have performed SXRMS measurements on a magnetically modulated, but chemically homogenous, Ni layer in a Cu/Ni/Cu system. Although this is both structurally and magnetically a rather complicated system for scattering studies, the preliminary data analysis looks very promising. Specular rod scans were used to study the structural profile of the sample. The oscillations owing to Kiessig fringes observed in the specular rod scans with different photon energies in the vicinity of the element-specific absorption edges allowed us to determine the corresponding layer thicknesses of the sample. However, at low angles an extra dip in the reflectivity is observed that does not appear in the case of multilayers with in-plane homogeneity. We ascribe this extra feature to interference from the in-plane periodicity in the sample.

Rocking scans were used to study the in-plane periodicity of the sample. Diffraction peaks are observed with a spacing of 0.0001 Å-1, corresponding to a periodicity of the wires of 6 µm. Scans taken near the critical angle, where the X-rays penetrate only the capping layer, are still revealing a periodicity. This suggests that also the Cu capping has an in-plane periodic structure, possibly owing to a different oxidation of the single-crystalline and polycrystalline regions. At higher Bragg angles we observe an array of diffraction peaks, clearly showing that the sample diffracts like a grating. At the resonance of the Ni L2,3 and Cu L2,3 edges the specular peak exhibits extra structure and all diffraction peaks have an additional shoulder on the left-hand side. We ascribe this to interference of the grating profile at different depths in the sample.

We have demonstrated the coexistence of in-plane and perpendicularly magnetized domains in the sample from the selectivity for the magnetization direction using [\sigma]-polarized and circularly polarized light. First, there is a difference in the Ni L2,3-edge specular reflection after aligning the magnetization of all domains in-plane using an applied magnetic field. Second, the MCD in the reflectivity is different for the coexisting magnetic domain configuration and the in-plane magnetic configuration.

The magnetic depth profile was measured by the MCD in reflectivity. At the Ni L3 resonance energy the Kiessig fringes in the specular rod scan are strongly suppressed compared with those at the Ni L2 energy owing to the reduced X-ray penetration length. The asymmetry ratio in reflectivity across the Ni L2,3 edge is very strong, showing a wealth of detailed structure. The spectral changes as a function of Bragg angle are remarkably strong.

A more quantitative analysis would be required to explore in detail the in-plain chemical and magnetic arrangement as well as the interdomain roughness. Calculations are in progress and will be presented in the near future.

Acknowledgements

We thank K. Larsson, P. Bencok and N. B. Brookes for their expert experimental assistance on the beamline.

References

First citationAlders, D., Hibma, T., Sawatzky, G. A., Cheung, K. C., van Dorssen, G. E., Padmore, H. A., Roper, M. D., van der Laan, G., Vogel, J. & Sacchi, M. (1997). J. Appl. Phys. 82, 3120–3124. CrossRef CAS Web of Science
First citationAls-Nielsen, J. & McMorrow, D. (2000). Elements of Modern X-ray Physics. New York: Wiley.
First citationBland, J. A. C., Lew, W. S., Li, S. P., Lopez-Diaz, L., Vaz, C. A. F., Natali, M. & Chen, Y. (2002). J. Phys. D, 35, 2384–2390. Web of Science CrossRef CAS
First citationChesnel, K., Belakhovsky, M., Landis, S., Rodmacq, B., Dudzik, E., Collins, S. P., Dhesi, S. S. & van der Laan, G. (2001). IEEE Trans. Magn. 37, 1661–1663. Web of Science CrossRef CAS
First citationChesnel, K., Belakhovsky, M., Landis, S., Toussaint, J. C., Collins, S. P., van der Laan, G., Dudzik, E. & Dhesi, S. S. (2002). Phys. Rev. B, 66, 024435/1–9.  CAS
First citationCowburn, R. P., Adeyeye, A. O. & Bland, J. A. C. (1997). Appl. Phys. Lett. 70, 2309–2311. CrossRef CAS Web of Science
First citationDaillant, J. & Gibaud, A. (1999). X-ray and Neutron Reflectivity: Principles and Applications, Lecture Notes in Physics 58. Berlin: Springer.
First citationDhesi, S. S., Mirone, A., De Nadai, C., Ohresser, P., Bencok, P., Brookes, N. B., Reutler, P., Revcolevschi, A., Tagliaferri, A., Toulemonde, O. & van der Laan, G. (2004). Phys. Rev. Lett. 92, 056403/1–4.  Web of Science CrossRef CAS
First citationDudzik, E., Dhesi, S. S., Dürr, H. A., Collins, S. P., Roper, M. D., van der Laan, G., Chesnel, K., Belakhovsky, M., Marty, A. & Samson, Y. (2000). Phys. Rev. B, 62, 5779–5785. Web of Science CrossRef CAS
First citationDürr, H. A., Dudzik, E., Dhesi, S. S., Goedkoop, J. B., van der Laan, G., Belakhovsky, M., Mocuta, C., Marty, A. & Samson, Y. (1999). Science, 284, 2166–2168. Web of Science CrossRef PubMed CAS
First citationEbels, U., Radulescu, A., Henry, Y., Piraux, L. & Ounadjela, K. (2000). Phys. Rev. Lett. 84, 983–986. Web of Science CrossRef PubMed CAS
First citationHannon, J. P., Trammell, G. T., Blume, M. & Gibbs, D. (1988). Phys. Rev. Lett. 61, 1245–1248. CrossRef PubMed CAS Web of Science
First citationJaouen, N., Tonnerre, J. M., Raoux, D., Bontempi, E., Ortega, L., Muenzenberg, M., Felsch, W., Rogalev, A., Dürr, H. A., Dudzik, E., van der Laan, G., Suzuki, M. & Maruyama, H. (2002). Phys. Rev. B, 66, 134420/1–14.  Web of Science CrossRef CAS
First citationKao, C.-C., Chen, C. T., Johnson, E. D., Hastings, J. B., Lin, H. J., Ho, G. H., Meigs, G., Brot, J.-M., Hulbert, S. L., Idzerda, Y. U. & Vettier, C. (1994). Phys. Rev. B, 50, 9599–9602. CrossRef CAS Web of Science
First citationKrusin-Elbaum, L., Shibauchi, T., Argyle, B., Gignac, L. & Weller, D. (2001). Nature (London), 410, 444–446. Web of Science PubMed CAS
First citationLaan, G. van der (1999). J. Magn. Magn. Mater. 192, 297–304.
First citationLaan, G. van der, Dudzik, E., Collins, S. P., Dhesi, S. S., Dürr, H. A., Belakhovsky, M., Chesnel, K., Marty, A., Samson, Y. & Gilles, B. (2000). Physica B, 283, 171–174.
First citationLaan, G. van der, Dürr, H. A., Dudzik, E., Roper, M. D., Collins, S. P., Hase, T. P. A. & Pape, I. (1999). Synchrotron Rad. News, 12(3), 5–9.
First citationLaan, G. van der & Thole, B. T. (1991). Phys. Rev. B, 43, 13401–13411. CrossRef Web of Science
First citationLi, S. P., Lew, W. S., Bland, J. A. C., Lopez-Diaz, L., Vaz, C. A. F., Natali, M. & Chen, Y. (2002). Phys. Rev. Lett. 88, 087202/1–4.  CAS
First citationLovesey, S. W. & Collins, S. P. (1996). X-ray Scattering and Absorption by Magnetic Materials. Oxford University Press.
First citationO'Brien, W. L. & Tonner, B. P. (1994). Phys. Rev. B, 49, 15370–15373. CrossRef CAS Web of Science
First citationSacchi, M. & Mirone, A. (1998). Phys. Rev. B, 57, 8408–8415. Web of Science CrossRef CAS
First citationSève, L., Jaouen, N., Tonnerre, J. M., Raoux, D., Bartolomé, F., Arend, M., Felsch, W., Rogalev, A., Goulon, J., Gautier, C. & Bérar, J. F. (1999). Phys. Rev. B, 60, 9662–9674. Web of Science CrossRef CAS
First citationTaniyama, T., Nakatani, I., Namikawa, T. & Yamazaki, Y. (1999). Phys. Rev. Lett. 82, 2780–2783. Web of Science CrossRef CAS
First citationThole, B. T., Carra, P., Sette, F. & van der Laan, G. (1992). Phys. Rev. Lett. 68, 1943–1946. CrossRef PubMed CAS Web of Science
First citationTonnerre, J. M., Sève, L, Barbara-Dechelette, A., Bartolomé, F., Raoux, D., Chakarian, V., Kao, C. C., Fischer, H., Andrieu, S. & Fruchart, O. (1998). J. Appl. Phys. 83, 6293–6295. Web of Science CrossRef CAS

© International Union of Crystallography. Prior permission is not required to reproduce short quotations, tables and figures from this article, provided the original authors and source are cited. For more information, click here.

Journal logoJOURNAL OF
SYNCHROTRON
RADIATION
ISSN: 1600-5775
Follow J. Synchrotron Rad.
Sign up for e-alerts
Follow J. Synchrotron Rad. on Twitter
Follow us on facebook
Sign up for RSS feeds